B. The foam core of the panel has internal indentations.
Foam Core Depression in Sheet Materials
Foam core depression is a common problem in the production of XPS, EPS, and PET extruded sheets. We offer the following solutions for different causes:
1. Melt temperature is too low: Increase the material temperature and the temperature of the main extruder (single screw).
2. The mold structure is not suitable for producing sheets of this thickness: Replace the mold and select a more suitable flow channel.
3.Mold temperature is too low: Gradually increase the mold temperature in increments of 3℃ to 5℃ each time.


Leave Message:
Please provide valid contact information.
We will offer free samples with TDS/MSDS.
Contact Us
KARJIA Polymer Material Tech Limited
Tel:+86 139 6843 1127 Mr.lin
Tel:+86 139 2252 5034 Mr.lin
Fax:+852 2134 9732
Technical / Product service Email:
servicelin@xpsmate.com
servicechen@xpsmate.com
Product consultation service Email :
info@xpsmate.com
Complaint Email :complaints@xpsmate.com
Tel/whatsapp:+86 139 6843 1127